Most welding problems we are asked about are not machine problems. They are fit-up problems, gas problems, or expectations set by a video of someone welding two clean plates on a bench. What follows are the notes we hand to buyers before a handheld or platform welder leaves Foshan — one material at a time, in the order these issues actually show up.

Stainless steel: the easy case, until it isn’t

304 and 316 weld cleanly at 1,000–1,500 W with a 0.8–1.2 mm spot and argon shielding. On 1–3 mm sheet, a handheld unit at 1,200 W with 3–4 mm overlap per pass gives a bead that needs no polishing on a brushed finish. Two things go wrong most often: no gas pre-flow, which leaves a grey start dot, and too much power for the sheet, which produces a keyhole that closes with a sink at the end of the seam. Both are settings habits, not equipment limits. If your parts are 0.5 mm foil or 8 mm plate, the same machine needs a different lens and a different motion, and it is worth saying so before you order.

Aluminium: power, speed and the oxide layer

Aluminium reflects roughly 90 % of a 1,070 nm beam cold and drops to about 70 % once the keyhole opens, so the first millimetres are always the hard part. On 2–4 mm 6061, 1,500 W with a 1.0 mm spot, 60–80 mm/s and argon works; below 1,000 W you fight lack of penetration rather than reflection. The surface oxide melts at around 2,000 °C while the metal underneath melts at 660 °C, which is why a wire feed or a slightly defocused first pass helps on thick sections. Clean the oxide with a stainless brush, not a grinding disc — grinding smears aluminium across the surface and gives you porosity that looks like a gas problem.

Copper and brass: the case for higher power

Copper is where 1.5 kW stops being comfortable, 2 kW starts earning its price, and 3 kW is where thick copper and long seams stop being a question. Thin copper — busbar tabs, heat-pipe joints, 0.5–1 mm — will weld at 1,500 W if the part is clean and the fixture holds it flat, but expect a narrow process window: a little more speed and you get lack of fusion, a little less and you get spatter. Brass is easier than pure copper but zinc evaporates and leaves a white deposit around the seam; that is normal, and it needs ventilation rather than a setting change.

Galvanised and coated steel

Zinc boils at 907 °C, well below the steel melting point, so the coating becomes gas inside the weld pool. The result is porosity and a popping sound. Two practical answers: weld in a lap joint rather than a butt so the zinc can escape at the gap, or remove the coating within 10–15 mm of the seam. Neither is free — this is the one material where we tell buyers to test their own parts before choosing a machine.

Fixtures matter more than watts

Laser welding has a very small heat-affected zone, which means it does not correct bad fit-up the way arc welding does. A 0.2 mm gap on 1 mm sheet shows up as a seam that is half width. On the platform machines we sell, the clamping table and the travel axis usually decide the result more than the source does; on handheld units, a steady rest and a second pair of hands matter just as much. If you are welding a repeated part, budget for a fixture before you budget for extra power.

What the numbers on the datasheet do not tell you

Peak power, spot size and feed rate are all real, but the useful figure is the one you get after ten minutes of continuous welding on your own part: does the head stay cool, does the chiller hold temperature, does the wire feed stay consistent. That is why we test-run every welder for at least 30 minutes on scrap from the customer’s own material before it ships, and why we ask for a sample part when the material is unusual. Send us a photo of the joint and the thickness and we will tell you whether 1.5 kW is enough — and if it is not, we will say so.